Refractory materials used in the regenerators of glass furnaces
Date:2016-04-25 17:32 From:Zhengzhou Sunrise Refractory Author:sunrise
Part name | Requirements | Varieties | |
Upper crown | Feeding port | One side heated, good resistance to high temperature, flying ash and alkali vapor | Direct bonding magnesia chrome brick or fused cast AZS brick or silica brick |
Backend | Good resistance to alkali vapor | Silica brick | |
Sidewall | Upper layer | Good resistance to dust and alkali vapor | Iron wrapped magnesia chrome brick or fused cast AZS brick |
Middle layer | No reaction with the upper basic bricks | Low porosity fire clay brick | |
Lower part | High strength to resist the low temperature and spalling | Fire clay brick | |
Internal separation walls | Upper layer | High-temperature strength, good resistance to creep and corrosion by dust and alkali vapor | Direct bonding magnesia chrome brick or silica brick |
Middle layer | Good resistance to creep and corrosion by alkali vapor | Direct bonding magnesia chrome brick or low porosity fire clay brick | |
Lower part | High strength to resist the middle temperature and spalling | Low porosity fire clay brick | |
Checker work |
Top layer >1300℃ |
Good resistance to high temperature, flying ash and alkali vapor | Direct bonding magnesia brick |
Cross-shaped AZS brick | |||
Upper layer >1100℃ |
Sintered magnesia brick | ||
Cross-shaped AZS brick | |||
Middle layer (Upper part) |
High temperature strength, good creep resistance | Sintered magnesia chrome brick | |
Cross-shaped AZS brick | |||
Middle layer (Lower part) |
High strength to resist the middle temperature, good corrosion resistance to Na2SO4, prevent the curing of Na2SO4 and damage caused by repeated liquefaction | Direct bonding magnesia chrome brick | |
Cross-shaped AZS brick | |||
Lower layer | No reaction with basic bricks, sufficient strength to resist the middle temperate | Low porosity fire clay brick | |
Cross-shaped AZS brick | |||
Rider arch | Good strength to resist the low temperate, good creep resistance | Low porosity fire clay brick |
Send an Inquiry
E-mail : sales@sunriserefr.com
Phone : +86-371-63838939 / Fax:+86-371-63835539
Company Address : No.36 Fengchan Road Of Zhengzhou, Henan, China (Mainland)
If you have any needs our help or are interested in our products, you can click online advisorychat with us online, or call our customer service telephone: 0086-0371-63838939. We will sincerely serve for you!
Product Category
- Fused Cast AZS
- Fused Cast AZS Block
- Fused Cast Skid Rail Block
- Fused Cast High Zirconia Block
- Fused Cast AZS Block
- Fiber Products
- Insulation Series Brick
- Fireclay Brick
- High Alumina Brick
- Corundum Brick
- Sillimanite Brick
- Mullite Brick
- Zircon Mullite Brick
- Zircon Brick
- Magnesia Brick
- Silica Brick
- Fused Cast Alumina Block
- Glass Mould Brick
Refractory Knowledge
moreCase
-
UAE to our factory inspection bri
...
-
Venezuela customer AZS fused bric
Venezuela customer AZS fused float glass furnace br...